Me pehea te whakapai ake i nga waahanga whakarakei o te reiti whakahekeheke
Ko te taumata spheroidization o te kaainga noa o te whare wira graphite maka whakarewa putunga e hiahiatia ana kia eke ki te taumata 4 ki runga atu ranei, (ara, ko te 70% te reanga o te spheroidization), ko te tere o te spheroidization i tutuki i nga papaanga whanui mo te 85%. I nga tau kua taha ake nei, me te whakawhanaketanga o te hanga rino hanga nodular, ina koa i roto i nga umanga me nga whakaritenga nui mo te hanga mana hiko hau me te kounga whakaheke, e hiahiatia ana te taumata whakahirahira kia eke ki te taumata 2, ara, ko te tere o te spheroidization kua eke ki te 90%. I tarai te kamupene a te kaituhi me te whakapai ake i te mahi spheroidization me te inoculation i whakamahia i QT400-15, me te kaihoko spheroidizing me te inoculant, kia tae ai te tere spheroidization o nod iron cast iron neke atu i te 90%.
1. Te mahinga whakaputa taketake
Tukanga whakaputa taketake:
- Ko nga taputapu smelting ka mau ki te oumu auau takawaenga 2.0T me te oumu ahumahi auau 1.5T;
- Ko te hanganga o te QT400-15 waikawa rino mata ω (C) = 3.75% ~ 3.95%, ω (Si) = 1.4% ~ 1.7%, ω (Mn) -0.40%, ω (P) -0.07%, ω ( S)) ≤0.035%;
- Ko te kaihoko spheroidizing e whakamahia ana i te maimoatanga spheroidizing he 1.3% ki te 1.5% RE3Mg8SiFe koranu;
- Ko te inoculant e whakamahia ana i te rongoa inoculation ko te 0.7% ~ 0.9% 75SiFe-C koranu. Ko te maimoatanga spheroidizing e tango ana i nga tikanga e rua mo te patuki me te pupuhi:
Tuatahi, 55% ~ 60% o te rino ka whakaputahia, katahi ka mahia te spheroidizing, katahi ka tapirihia te inoculant, katahi ka tapirihia te toenga o te wai rino.
Na te tikanga tuku iho mo te spheroidization me te inoculation, ko te tere spheroidization e kitea ana e te poraka whakamatautau kotahi poro me te matotoru o te 25 mm te nuinga o te 80%, ara, ko te taumata spheroidization ko te 3.
2. Mahere mahere hei whakapai ake i te reiti whakahekeheke
Kia pai ake ai te reiti o te spheroidization, kua pai ake te mahi whakaohooho tuuturu me te taatai. Ko nga mahinga matua: ko te whakapiki i te nui o te kaihoko spheroidizing me te inoculant, te whakarewa i te rino rewa, me te whakamaimoatanga kore. Ko te reanga spheroidization kei te whakamatautauria tonu me te poraka whakamatautau kotahi poro 25 mm. Ko te mahere ake e whai ake nei:
- (1) Te wetewete i te take mo te reeti iti o te mahi taketake. I whakaarohia ko te rahinga o te kaihoko spheroidizing he iti, no reira ko te nui o te kaihoko spheroidizing kua taapirihia i piki ake mai i te 1.3% ki te 1.4% ki te 1.7%, engari kaore i tutuki i te reanga spheroidizing nga whakaritenga. . (2) Ko tetahi atu whakapae ko te iti o te utu mo te spheroidization na te ngoikore o te tohu whakaheke, te heke ranei o te huautanga. Na reira, i whakapiki ake te whakamatautau i te horopeta whakauru mai i te 0.7% ki te 0.9% ki te 1.1%, a, kaore i tutuki i te tere spheroidization nga whakaritenga.
- (3) Taria tonu ki te tarai me te whakapono he nui ake nga whakauru o te rino rewa me te nui o te aukatinga o te spheroidization ko nga take pea o te reiti iti o te spheroidization. No reira, ko te whakamahana teitei o te rino whakarewa o te rino whakarewa ka mahia. Ko te pāmahana horoi teitei-pāmahana te tikanga kei te whakahaerehia i te 1500 ± 10 ° C, engari Ko tana reanga whakaoringa kaore i neke atu i te 90%.
- (4) Ko te nui o te ω (S) e tino whakapau ana i te horopeta spheroidizing me te whakatere i te heke o te spheroidization. No reira, kua whakapikihia te maimoatanga desulfurization ki te whakaheke i te wai rino taketake ω (S) mai i te 0.035% ki te iti iho i te 0.020%, engari ko te utu mo te spheroidization kua tae noa ki te 86%. Ko nga hua whakamatautau o nga kaupapa e wha i runga ake nei e whakaatuhia ana i te Ripanga 1. Ko nga hanganga me nga miihini o te poraka whakamarama ahua-poro kaore i tutuki nga whakaritenga.
3. Te mahere whakapai ake whakamutunga i tangohia
3.1 Nga whakaritenga whakapai ake
- Ko nga mea mata ko te rino poaka, he waikura, he iti ake ranei te waikura waikuraki me nga mea whakaranu;
- Te whakamaarama i te rino rewa reima ma te taapiri i te pungarehu houra (Na2CO3) ki te oumu;
- Whakamahia te kaihoko whakahoahoa Foseco 390 hei whakakaha-i-mua i roto i te peke;
- Maimoatanga Spheroidizing me Fozco Nodulizer;
- Te whakamahi i te karapoti silicon me te ferrosilicon inoculation honohono.
Ko te mana hanga whakarewa whakarewa taketake o te mahinga hou: ω (C) = (3.70% ~ 3.90%, ω (Si) = 0.80% ~ 1.20% [maka ana ω (Si whakamutunga) = 2.60% ~ 3.00%], ω ( Mn) ≤ 0.30%, ω (P) ≤0.05%, ω (S) ≤0.02%. Ka nui atu te rino whakarewa taketake ω (S) ki te 0.02%, ka whakamahia te pungarehu houra umanga mo te whakakorenga i mua o te oumu, na te mea Ko te tauhohenga desulfurization he tauhohenga endothermic, Ko te pāmahana desulfurization me whakahaere i te taha o 1500 ° C, a ko te rahinga houra pungarehu kua taapirihia e whakahaerehia ana i te 1.5% ~ 2.5% e ai ki te nui ω (S) i te wa e rewa ana i te oumu .
I te wa ano, ko te kohinga maimoatanga spheroidizing ka tango i tetahi kohinga maimoatanga momo waipuke noa. Tuatahi, taapirihia te 1.7% o te kaihoko Foseco NODALLOY7RE tohu kaihoko mo te taha o te poka i raro o te kete, whakahiato me te kiato, ka whakamahi i te 0.2% paura karaka silicon puehu me te 0.3% iti Ko te tini 75SiFe ka kapi ki tetahi papanga tetahi i muri o tetahi. , ana, ka oti te whakaweto, ka kapi ki te rino pehanga, ana ka honoa te 0.3% Foseke 390 inoculant ki tera taha o te riini rino whakarewa. A, no te taatai i te rino, 55% ~ 60% o te tapeke o te rino rewa i whakarewahia i te tuatahi. I te otinga o te tauhohenga spheroidizing, 1.2% 75SiFe-C inoculant ka taapirihia ka toeahia te toenga rewa rewa, ka riringihia te para.
3.2 Nga whakamatautau
Ko te hanganga o te rino rewa whakarewa i mua atu i muri hoki i te whakakorenga, nga miihini miihini me te anga whakarewa o te 25mm poraka whakamatautau kotahi-poraka, me te tikanga aromautanga o te reiti spheroidization i roto i te hanga whakarewa whakariterite ka kitea noa e te punaha tarai whakaahua whakarake .
4. Te wetewete hua
4.1 Te awe o nga mea matua ki te utu mo te spheroidization
- C, Si: Ka taea e C te whakatairanga i te whakairoiro me te whakaiti i te haangai o te waha ma, engari ko te nui o te ω (C) ka teitei rawa atu ai te CE, ka ngawari ai te rere o te kauwhata, 3.7% ~ 3.9% te tikanga. Ka taea e Si te whakakaha i te aahua whakairoiro me te whakakore i te sima. Ka tapirihia a Si hei inoculant, ka taea te whakaheke i te kaha o te rino rewa. Hei whakapai ake i te paanga o te weronga, ka heke te nui o te ω (Si) i te rino whakarewa taketake mai i te 1.3% ki te 1.5% ki te 0.8% ki te 1.2%, me te rahinga ω (Si whakamutunga) i whakahaerehia i te 2.60% ki te 3.00%.
- Mn: I te wa o te mahinga whaanui, ka whakanui te Mn i te whakarewa o te rino ki te kapi me te whakatairanga i te hangai o nga waikura (FeMn) 3C. I roto i te huringa huringa eutectoid, ka whakaitihia e te Mn te mahana o te huringa eutectoid, ka whakapumau ka whakamahine i te peara. Kare he awe o te Mn ki te reanga o te spheroidization. Na te awe o nga rauemi mata, te tikanga whakahaere ω (Mn) <0.30%.
- P: I te ω (P) <0.05%, he totoka-wairewa i roto i te Fe, a he uaua ki te hanga i tetahi phutoro eutectic, he iti nei te awe ki te tere spheroidization o te rino koretake.
- S: Ko te S he mea whakararu kore. Ka pau i te S te Mg me te RE i roto i te kaihoko spheroidizing i te wa o te urupare spheroidizing, me te aukati i te whakaorititanga me te whakaiti i te tere spheroidizing. Ka hoki ano te waikura Sulphide ki te whanariki i mua i te whakakotahi o te rino rewa, ka pau ano i nga waahanga o te spheroidizing, te whakatere i te paheketanga o te spheroidization, ka pa ano ki te tere o te spheroidizing. Kia tutuki ai te tere o te spheroidization, ko te rahinga o te ω (S) o te rino mata me heke ki raro iho i te 0.02%.
4.2 Maimoatanga Desulfurization
I muri i te rewa o te utu, tirohia nga tauira ka taatai i te waahanga matū. Ki te nui ake te rahinga ω (S) i te 0.02%, me whakakorekore te mahi.
Ko te kaupapa o te pungarehu pungarehu houra ko te: whakatakotoria he pungarehu houra ki te koko, whakamahia he reini rewa ki te piu me te whakaohooho, te pungarehu pungarehu e pirau i te teitei o te mahana, ko te whakautu urupare Na2CO3 = Na2O + CO2 ↑: ko te Na2O i hangaia i roto i te rino rewa ano Te Whanariki me te hanganga o Na2S, (Na2O) + [FeS] = (Na2S) + (FeO).
Na2CO3 ka wehe ka whakatau i a CO2, na te tutu o te rino rewa, he whakatairanga i te mahi desulfurization. He ngawari te rere o te pungarehu houra ki te rere ka tere tere, ana he poto rawa te wa urupare desulfurization. I muri i te whakakoretanga, me tango te otaota i te wa tika, mena ka hoki ano ki te whanariki. 4.3 Maimoatanga i mua i te whakakorenga, maimoatanga spheroidization me te rongoa inoculation Ka whakamahia e te kaihoko whakairo o te Foseke 390 te rongoa i mua i te deoxidation i roto i te peke, a i te wa ano ka whakapiki ake i te kaupapa matua o te karahipi me te maha o nga mata kauwhata i ia waahanga waahanga, ka taea hoki whakapiki i te tere o te ngongo o te Mg. Whakapai ake i te kaha ki te aukati i te pahekeheke me te whakanui ake i te reiti whakahekeheke. Ko te Inoculant o Fochke kei roto ω (Si) = 60% ~ 70%, ω (Ca) = 0.4% ~ 2.0%, ω (Ba) = 7% ~ 11%, a ka taea e Ba te whakaroa i te waa whakaurunga whaihua. Ko te kohinga NODALLOY7RE o Fozco Nodulizer kua tohua, me tana ω (Si) = 40% ~ 50%, ω (Mg) = 7.0% ~ 8.0%, ω (RE) = 0.3% ~ 1.0%, ω (Ca) = 1.5 % ~ 2.5%, ω (Al) <1.0%. Mai i te rino rewa e uru ana ki te whakakorenga o te tangata me nga maimoatanga o mua-deoxidation, ko nga mea e kai ana i nga nodulizers i roto i te rino rewa kua tino heke, no reira ka tohua he nodulizer me te iti o te ω (RE) hei whakaheke i te tino kino o te aorangi graphite spheroidal na RE. ; Ko te kaupapa matua o te mahi ko te Mg; Ka taea e Ca me Al te mahi ki te whakapakari ake i te aarai. Ma te whakamahi i te silicon carbide me te ferrosilicon i roto i te rongoa inoculation, ko te ngako rewa o te silicon carbide e tata ana ki te 1600 ° C, ka whakapikihia te karihi karihi karaamiti i te wa e pakari ana, a ka whakamahia nga waahanga nui o te ferrosilicon mo te weronga, ka aukati i te whakahekenga o te spheroidization.
Whakamutunga 5
I roto i te hanga rino uira nehu ferular, ka hiahiatia te tere spheroidization kia neke atu i te 90%, ka taea nga mahi e whai ake nei:
- (1) Tiwhiria te utu kounga-pai hei whakaiti i nga waahanga de-spheroidization kei roto i te utu.
- (2) Tiwhiria tetahi kaihoko spheroidizing me te iti o te ω (RE) hei whakaiti i te kino kino o te RE ki te whakaaturanga o te kauwhata Spheroidal.
- (3) Ko te ω (S) o te rino whakarewa taketake kia iti ake i te 0.020%, ka taea te whakaiti i te kohi o nga nodulizer, ina koa ko nga waahanga nodulized kua pau i te sulfurization tuarua o te otaota sulfide.
- (4) I mua i te whakakore i te rino rewa, whakarahi ake i nga waahanga graphite mo ia waahanga waahanga, whakanui ake i te tere o te spheroidization, te whakapai ake i te kaha ki te aukati i te paheke o te heke, me te whakaroa i te waa whakaohoa whaihua.
- (5) Whakaitihia te of (Si) ki te rino whakarewa taketake, whakapiki i te kaihoko spheroidizing, inoculant me nga momo momo kaitohu, me te whakakaha i te rongoa rongoa.
Tena koa kia mau ki te maataapuna me te wahitau o tenei tuhinga mo te taarua: Me pehea te whakapai ake i nga waahanga whakarakei o te reiti whakahekeheke
Minghe Kamupene Tika Raka e whakatapua ana ki te hanga me te whakarato i te kounga me te mahi nui mo te whakangao i nga waahanga (ko nga waahanga whakarewa mate whakarewa te nuinga o te waa Te Maka i te Mate Maehe-Tutuki,Te Horo Hou o te Ruma wera,Te Makarekare Whare Toi Toto), Ratonga Rauna (Ratonga Maka Mate,Miihini Cnc,Hanga Whakatika, Maimoatanga Mata). Ko nga tohu Alumini kua mate, he konupora, he Zamak / zinc / casting zinc ranei, me etahi atu whakaritenga maka e manakohia ana kia whakapiri mai ki a maatau.
I raro i te mana whakahaere o te ISO9001 me te TS 16949, ko nga mahinga katoa ka mahia i roto i nga miihini miihini whakaheke rau, miihini 5-tuaka, me etahi atu taputapu, mai i nga miihini ki nga miihini horoi horoi Ultra Sonic. roopu o nga kaiwhakangungu mohio, kaiwhakahaere me nga kaitirotiro kia pono te hoahoa a te kaihoko.
Kaihanga kirimana mo te whakaheke mate. Ko nga kaitautoko kei roto i te whare matao konumohe e mate ana i nga waahanga mai i te 0.15 lbs. ki te 6 lbs., ka whakatauhia te whakarereke tere, me te miihini. Ko nga ratonga e taapirihia ana ko te oro, te wiri, te pahekeheke, te pupuhi pupuhi, te peita, te whakakikorua, te paninga, te huihuinga, me te taputapu. Ko nga rauemi i mahi ngatahi ai ko nga kikii puri penei i te 360, 380, 383, me te 413.
Zinc mate casting hoahoa awhina / ratonga hangarau rite. Kaihanga Ritenga o te whakakautei te mate konutea. Te whakaheke i te Iti, te whakaheke i te peehi teitei, te whakaheke i te miihini maha, te miihini miihini tikanga, te mate o te waahanga me te whakaheke i te mate motuhake me te tohu o te kohao kua oti te hiri. Ka taea te hanga Castings i te roa me te whanui tae atu ki te 24 in. I roto i te +/- 0.0005 in. Manawanui.
ISO 9001: 2015 kaiwhakanao tiwhikete o te konupora maka mate, Ko nga kaha kei roto i te konupora teitei e mate ana kia tae atu ki te 200 tana ruuma wera & 3000 tana teena makariri, hoahoa taputapu, oroina, whakarewa, miihini, paura me te peita wai, QA katoa me nga kaha CMM , huihuinga, takai me te tuku.
ITAF16949 tiwhikete. Ratonga Maka Maka Taapiri Tae Atu te haumi haumi,whakarewa kirikiri,Ngakau Kari, Ngaro Kamupene ngaro,Peke Uru,He Kai Ware,Te Maka Mould Tuturu, .Mahinga he EDI, awhina hangarau, whakatauira totika me te tukatuka tuarua.
Nga Mahi Maka Maka Nga Wahanga Akoranga mo nga: Motuka, Pahikara, Papa rererangi, taonga puoro, Waiwai, taputapu Optical, Sensors, Tauira, taputapu Hiko, Whakapiringa, Karaka, Miihini, Miihini, Taonga, Taonga, Taimana, Telecom, Rama, Taputapu Hauora, taputapu Whakaahua, Karetao, Whakaahua, Taputapu Oro, Taputapu Hakinakina, Taputapu, Taonga me etahi atu.
He aha ta maatau hei awhina i a koe a muri atu?
∇ Haere ki te Wharangi Kaainga Mo Mate Maka Makaina
→Wahanga Taputapu-Rapua nga mahi i mahia e maatau.
→ Tohu Awhina mo te Mate Ratonga Maka
By Minghe Die Casting Kaihanga | Kāwai: Tuhinga Tauturu |Rauemi Tags: Tini Panuiini, Maka Maka, Makaora Maka, Te Maka Titanium, He kowiriira Casting, Maka Maka,Te Maka Koura,Whakaari Ataata,Hītori Kamupene,Porohita Mate Paratini | Korero Kore